Epoxy Prepregs : Ep-preg®
Ep-preg® pepregs are highly suitable for vacuum curing process, are especially designed to be in a B- Stage for at least 3 months@ 20-23°C, and cure within 120 min.@ 121° C. Ep-preg S153 has been qualified for Wind Blade manufacturing.
Specific uses
Ep-preg® | Applications |
---|---|
Bisphenol A type | |
S153 |
|
Fire Retardant | |
F64-A1 |
|
Toughened Bisphenol A type | |
T353 T433 |
|
Technical specifications
Product Name | Resin Type | Fiber | Product Form® and FAW(gsm) | DSC Tg(°C) | Months @RT | Gel Time (mins) | Recommended cure | Market/Applications |
---|---|---|---|---|---|---|---|---|
Ep-Preg® S153 | Epoxy (Bisphenol A) | SM Carbon E-Glass | Fabric and Stiched UD (200-1600) | 115 | 2-3 | 25-30@100°C 7-9@120°C | 6h@100°C 2h@120°C | Wind Blades, Industrial |
Ep-Preg® F64-A1 | Epoxy (Fire-Retardant) | SM CarbonE-Glass | Fabric and Stitched UD (200-650) | 115 | 2-3 | 25-30@100°C 7-9@120°C | 6h@100°C 2h@120°C | Mass-transit, Defense |
Ep-Preg® T353 | Epoxy (Toughened) | SM CarbonE-Glass | Fabric and Stitched UD (200-650) | 100 | 2-3 | 25-30@100°C 7-9@120°C | 6h@100°C 2h@120°C | Industrial |
Ep-Preg® T433 | Epoxy (Toughened) | SM CarbonE-Glass | Fabric and Stitched UD (200-650) | 130 | 1-2 | 60-100@90°C 6-9@ 120°C | 1h@90°C 2h@120°C | Aerospace, Industrial |
Ep-Preg® S883 | Epoxy (Bisphenol A) | SM CarbonE-Glass Aramid Basalt | 200-1200 | 125 | 3-4 | – | 1h@135°C +15min@150°C | Industrial |
Ep-Preg® T875 | Epoxy (Toughened Bis A) | SM CarbonE-Glass Aramid Basalt | 200-1200 | 125 | 5-6 | – | 1h@135°C +15min@150°C | Industrial, Sport & Leisure |
Ep-Preg® S933 | Epoxy (Modified Bis A) | SM CarbonE-Glass Aramid Basalt | 200-1200 | 170 | 6-8 | – | 1h@135°C +15min@175°C | Aerospace, Defense, Electronics |